Copper-titanium is the usual beryllium-free replacement for C17200 in small signal contacts and springs: it reaches 885 to 1,180 MPa with good bend formability. Stay with beryllium copper when the contact carries real current or needs the highest strength, because C17200 conducts two to three times better (22 to 28 % IACS against 8 to 13 %) and reaches about 1,500 MPa after age hardening.

Side-by-side data

C17200C1990YCuT-FX
UNSC17200C19900C19900
EquivalentsEN CuBe2 / CW101C; JIS C1720; GB QBe2 (TBe2)JIS C1990; EN CuTi3JIS C1990
Composition %Be 1.80 – 2.00, Co + Ni ≥ 0.20, Co + Ni + Fe ≤ 0.60Ti 2.9 – 3.5Ti 3.2
Conductivity %IACS22 – 288 – 1313
Tensile strength MPa410 – 1520885 – 1180985 – 1115
TempersA (TB00), 1/4H (TD01), 1/2H (TD02), H (TD04), AT (TF00), 1/2HT (TH02), HT (TH04)EH, SH, ESHH, EH, SH, ESH
Elastic modulus131 GPa127 GPa125 GPa
Density8.25 g/cm³8.70 g/cm³8.7 g/cm³

Tensile strength is the range across supplied tempers. Full composition, tempers and physical properties are on each grade page.

Choose copper-titanium (C1990, YCuT-FX) when

Choose beryllium copper (C17200) when

Notes

YCuT-FX has the same basic composition as C1990 and is processed for a better balance of strength and bend formability in thin strip. Copper-titanium is supplied mill hardened. C17200 is available both mill hardened and in heat-treatable tempers.

Questions buyers ask

Is copper-titanium a drop-in replacement for beryllium copper?

Mechanically it is close in many spring designs, but the lower conductivity raises contact temperature under load. Check the current rating before switching.

Need a recommendation for a specific part?

Tell us the part function, strip thickness and performance targets. We reply within one working day, and sample coils are available for comparative trials.

Material development support