C5191 vs C5210 vs C5240: phosphor bronze grades compared

The three grades differ in tin content: about 6 %, 8 % and 10 %. More tin gives more strength and spring force and slightly less conductivity, at a higher price. C5191 is the general-purpose grade, C5210 is the standard spring grade, and C5240 is for miniature springs that need 850 MPa and above.

Side-by-side data

C5191C5210C5240
UNSC51900C52100C52400
EquivalentsEN CuSn6 / CW452K; JIS C5191; GB QSn6.5-0.1EN CuSn8 / CW453K; JIS C5210; GB QSn8-0.3JIS C5240
Composition %Sn 5.5 – 7.0, P 0.03 – 0.35, Cu + Sn + P ≥ 99.5Sn 7.0 – 9.0, P 0.03 – 0.35, Cu + Sn + P ≥ 99.7Sn 9.0 – 11.0, P 0.03 – 0.35, Cu + Sn + P ≥ 99.7
Conductivity %IACS13 – 15≈ 12≈ 11
Tensile strength MPa315 – 685470 – 885650 – 1000
TempersO, 1/4H, 1/2H, H, EH1/2H, H, EH, SH, ESHH, EH, SH, ESH, XSH
Elastic modulus110 GPa110 GPa105 GPa
Density8.83 g/cm³8.80 g/cm³8.78 g/cm³

Tensile strength is the range across supplied tempers. Full composition, tempers and physical properties are on each grade page.

Choose C5191 when

Choose C5210 when

Choose C5240 when

Notes

All three are solid-solution alloys hardened by rolling, so strength comes from the temper and no heat treatment is involved. Conductivity is low across the family, 11 to 15 % IACS, so phosphor bronze suits signal and low-current contacts.

Questions buyers ask

When is phosphor bronze not enough?

When the contact carries significant current or runs hot. A copper-nickel-tin or Corson alloy conducts three to four times better and relaxes less at temperature.

Need a recommendation for a specific part?

Tell us the part function, strip thickness and performance targets. We reply within one working day, and sample coils are available for comparative trials.